Popis: | The paper deals with abrasive waterjet titanium tangential turning. Titanium grade 3 with a diameter of 55 mm was used as an experimental material. Technological conditions of turning tests were the same by gradually changing value of traverse speed (vf = 1,5; 3; 4,5; 6; 7,5 mm・min-1). Experiment tests were performed by using continuous abrasive waterjet of pressure p = 400MPa, by rotation n = 60 rpm of workpiece. The abrasive particles (Barton Garnet) were fed to the waterjet in the amount of 0,4 kg・min-1. It was determined that acceleration of traverse speed did not increase the surface profile parameters. |