Popis: |
Polyamide epichlorohydrin (PAE) is a permanent wet strength resin. When applied to paperboard, some amount of resin is retained in the sheet, and some is lost to the white water. An analytical method for quantifying the amount of PAE retained in the sheet and lost into the white water has been developed. This method hydrolyzes the PAE to adipic acid, which in turn is derivatized to diethyl adipate and quantified by pyrolysis gas chromatography–mass spectrometry (pyGCMS). In addition, the hydrolysis conditions of the PAE were studied by the Taguchi approach, and PAE material balances around the dry sheet and white water for 3 and 6 lb/ton PAE applications have been performed. The PAE resin recovery was 95.4% with 65.0% in the sheet for the 3 lb/ton PAE-charged paper-board, and the recovery was 96.7% with 36.1% in the sheet for the 6 lb/ton PAE-charged paperboard. |