Torch guniting of open-hearth roof local burns.

Autor: Chemeris, O., Tsibin, I., Yusefovskii, I., Novikov, V., Korotkii, V., Savel'chikova, I., Kornienko, A., Bushnev, A., Kaduba, P., Chvilev, A., Malakhov, M., Chukhal', P.
Zdroj: Refractories; 1983, Vol. 24 Issue 5/6, p249-253, 5p
Abstrakt: The All-Union Institute for Refractories and Azov Steel Zhdanov Metallurgical Plant have developed a method of flame guniting of open-hearth roofs. Tests of this process conducted in 450-ton open hearths showed the possibility, in principle, of repairing local burns of periclase-spinellide roof refractories at the end of open-hearth campaigns. Torch guniting in open hearths provided a periclase coating with a porosity of 20-30% and a thickness of up to 50 mm, strongly bonded to the periclase-spinellide roof parts. The life of the coating on the roof is up to 10 heats. [ABSTRACT FROM AUTHOR]