Autor: |
Kaidash, O. N., Turkevich, V. Z., Ivzhenko, V. V., Itsenko, P. P., Tkach, V. N. |
Zdroj: |
Journal of Superhard Materials; Nov2018, Vol. 40 Issue 6, p365-373, 9p |
Abstrakt: |
A method of the reaction hot pressing was used to produce composites from the B4C-(5-15%)(TiH2-VC) system, established the peculiarities of their structures and measured physico-mechanical parameters. The dense dispersion-hardened materials having a high bending strength (Rbm = 420-580 MPa) and increased fracture toughness (KIc = 4.1-4.8 MPa·m1/2) on retention of the HKN = 19-20 GPa are promising for the use in the conditions of the severe abrasive wear. [ABSTRACT FROM AUTHOR] |
Databáze: |
Complementary Index |
Externí odkaz: |
|