Effect of the Deposition Direction on Fracture Propagation in a Duplex Stainless Steel Manufactured by Directed Energy Deposition
Autor: | David Roucou, Thomas Corre, Gilles Rolland, Véronique Lazarus |
---|---|
Přispěvatelé: | Institut des Sciences de la mécanique et Applications industrielles (IMSIA - UMR 9219), Commissariat à l'énergie atomique et aux énergies alternatives (CEA)-École Nationale Supérieure de Techniques Avancées (ENSTA Paris)-Université Paris-Saclay-Centre National de la Recherche Scientifique (CNRS)-EDF R&D (EDF R&D), EDF (EDF)-EDF (EDF), Institut de Recherche en Génie Civil et Mécanique (GeM), Centre National de la Recherche Scientifique (CNRS)-École Centrale de Nantes (Nantes Univ - ECN), Nantes Université (Nantes Univ)-Nantes Université (Nantes Univ)-Nantes université - UFR des Sciences et des Techniques (Nantes univ - UFR ST), Nantes Université - pôle Sciences et technologie, Nantes Université (Nantes Univ)-Nantes Université (Nantes Univ)-Nantes Université - pôle Sciences et technologie, Nantes Université (Nantes Univ)-Nantes Université - Institut Universitaire de Technologie Saint-Nazaire (Nantes Univ - IUT Saint-Nazaire), Nantes Université (Nantes Univ)-Nantes Université (Nantes Univ)-Nantes Université - Ecole Polytechnique de l'Université de Nantes (Nantes Univ - EPUN), Nantes Université (Nantes Univ)-Nantes Université (Nantes Univ), EDF R&D (EDF R&D), EDF (EDF), AID, CIEDS |
Rok vydání: | 2022 |
Předmět: | |
Zdroj: | Materials Science and Engineering: A Materials Science and Engineering: A, In press, ⟨10.1016/j.msea.2023.145176⟩ |
ISSN: | 1556-5068 0921-5093 |
Popis: | International audience; Dense volumes of duplex stainless steel are manufactured by directed energy deposition. Compact tension specimens are machined from these volumes in order to evaluate the fracture toughness in two directions : parallel or perpendicular to the deposited layers. Different values are measured in the two cases. In order to understand this anisotropy, additional analyzes are performed on the cracked specimens post-mortem. A classical metallography analysis reveals the highly oriented structure of the material, as well as phase localization. The study of the fracture surface reveals several points. At the macroscale, while the crack surfaces are flat in the parallel case, pronounced shear lips cover half of the fracture surface in the perpendicular case. At the microscale, fracture is ruled by microvoid coalescence. The mesoscale, which is inherited from the deposition strategy, is found to pilot the crack growth. The border between the primary solidified melt pools and the heat-affected zones, which corresponds to the interface between the deposited layers, is the preferred area for crack growth. Analyzing the crack surface roughness confirms the dominance of the mesoscale, as its characteristic lengthscale is retrieved. This explains the differences observed for the two tested directions of fracture: in the parallel case, the crack is aligned with the weak interfaces between layers, which channel the crack growth; in the orthogonal one, out-of-plane excursion of the crack becomes possible allowing the crack to follow a tortuous three-dimensional path that results in a higher toughness than in the parallel situation. |
Databáze: | OpenAIRE |
Externí odkaz: |