Popis: | It was shown that specimens with an open porosity below 3% can be produced from zircon wet-ground in a vibromill, treated with acid, and containing over 80% grains smaller than 10μ including 60–70% grains smaller than 2μ; the density of the specimens is highest (porosity below 1%) when they are fired at 1500°C and contain a maximum of 0.8–1% TiO2. |