Autor: |
Ponomareva, V. N., Kuzina, T. M., Yakovleva, V. S., Levin, A. M., Lavrov, I. S. |
Zdroj: |
Refractories; May 1984, Vol. 25 Issue: 5-6 p300-304, 5p |
Abstrakt: |
Conclusions The deposits in the study are multicomponent polydispersed suspensions characterized by a solid-phase concentration of 3.79–17.7% density 1–1.09 g/cm3, and a pH of 8.2–11.9. When the deposits are left to stand for 10 days they become compacted up to 40–70% of the original volume. The size of the aggregates of the dispersed phase change from 5 to 50 µm with a predominant particle size of 5 to 20 µm (64–79%). The electrokinetic potential of the phase is from -1.5 to -12.8 mV for various batches of deposits. |